Hull topsides
STEEL · ABOVE THE WATERLINEAlexseal High Solid basecoat and clearcoat over a Hempel corrosion primer and fairing base.
Outboard face
-
Alexseal HS Clear Coat H0150Second application. Optional, for a high-end finish. Reducer R5531 or R5561.45–60µm DFT
-
Alexseal HS Clear Coat H0150First application. 55 % volume solids, WFT 80–110 µm, recoat 24 h at 20 °C. Sand P320 within five to seven days and do not cut through to the basecoat. Tapes off within 24 h.45–60µm DFT
-
Alexseal HS Base Coat
H7153Light Gray70 % volume solids, WFT 40–80 µm, reducer R5521 or R5541. One cross coat gives full hide on greys. Recoat with clearcoat after tack-up, 3 to 24 h.20–40µm DFT -
Alexseal Finish Primer 44239 % volume solids, WFT 225–300 µm, reducer R4042 or R4032. Sand 320–400 on a DA. At least 50 µm must remain after sanding.90–120µm DFT
-
Alexseal Super Build 30260 % volume solids, WFT 350–900 µm, reducer R3040. Board sand 150, then 220 on a DA. At least 100 µm must remain after sanding.200–500µm DFT
-
Alexseal Fine Filler 303100 % solids, no reducer. As thin as possible, never more than 0.5 mm a layer. Sand 100–120 between coats, 120–150 before the next product.as thinas possible
-
Hempel fairing compoundPre-treatment and application to Hempel's own instruction.per Hempel
-
Hempel corrosion protection primerPre-treatment and application to Hempel's own instruction. Sand 80–120 and vacuum before the Alexseal system goes on.per Hempel
- SteelBlasted to Sa 2½, ISO 8501-1:2007. Stripe coat every edge, weld seam, stiffener and anything the spray gun cannot reach.
Substrate
- Conditions. 17 to 30 °C, 40 to 70 % relative humidity.
- Cure. Seven to ten days for Super Build 302, Finish Primer 442 and the basecoat and clearcoat.
- Tolerance. Final average DFT no less than 80 % and no more than 150 % of the figures above.
- Between every coat. Vacuum, optional freshwater rinse, then Alexseal Wipe Down Solvent by the two-cloth method with a minimum two-hour flash-off, then tack rags.